Recipe of Heating SGP Laminated Glass in EVA Vacuum Ovens
Following data is based on [6mmGLASS+0.76mmSGP+6mmGLASS], if you laminating thicker interlayer or glass, please keep the temperature, but prolong the holding time for both stages by 10-30mins.
1, Laminating room:
Temperature: 22°C - 28°C Humidity: 18% - 28%
2, Low temperature stage:
Cold vacuuming for 5 mins
10mins heating up to 65℃
Holding at 65℃ for 30mins
3, High Temperature stage
30mins heating up to 135°C
Holding at 135°C for 60mins
Cooling down at speed 3℃/min
Contact us, if you need help:
Peter Lin
Whatsapp: +86 15013829504
WeChat: wecan365